Most stick welding defects come from six causes: current set too high or too low, travelling too fast, holding too long an arc, damp rods, and dirty or coated metal. Read the bead, match the fault to its cause in the table below, change one thing at a time, and test a scrap before you weld the real job.

A gate hinge snaps at the toe of a weld. A trailer drawbar cracks a month after delivery. A water trough seeps through a line of pinholes you did not see under the paint. Each of these looked fine from the doorway, and each was a welding defect that the welder could have read in the bead and fixed on the day.

We already have guides to why a welder will not strike an arc and to choosing the right welding rod. This guide starts after the arc is running. It takes each defect in turn, shows what it looks like, what causes it, how to fix it, and how to test a weld in the workshop without special equipment.

How Do I Read a Weld Bead?

A good stick weld has a few simple signs. The bead is even in width, with fine, regular ripples like fish scales laid close together. It blends smoothly into the plates on both sides, with no groove cut along the edges. The slag lifts off easily, often by itself as the weld cools, and leaves a clean, bright surface with no holes.

A bad weld announces its fault the same way: a bead that is too tall and narrow, too flat and wide, lumpy, holed, or sitting on the plate like a line of glue. Before you reach for the amp dial, look at what the bead is telling you. The dial is the most common cause, but it is not the only one, and changing it blindly can swap one defect for another.

Defects by current setting What the Current Dial Does to the Bead Illustrative: conceptual scale, no figures from any one machine Current too low About right Current too high Rod sticks, arc stutters Tall, narrow bead Lack of fusion Slag trapped in the weld Steady crackle Even, fine ripples Smooth blend into plate Slag lifts off Rod glows, spatter Wide, flat bead Undercut along the edge Burn-through on thin metal Fix: raise the current Keep it here Fix: lower the current
Illustrative scale of how setting changes the look of the weld. Use the middle of the range printed on the rod packet as your starting point, then adjust by evidence.

What Causes Porosity, and How Do I Fix It?

Porosity is the family of small holes or pinholes in the weld. They are gas bubbles that were trapped as the metal froze. On the surface they show as pinholes or a foamy, honeycomb look. Inside, they can sit unseen in a row along the weld.

The usual causes are damp rods, a long arc, dirty or coated metal and moving too fast. A rod that has soaked up moisture releases steam and hydrogen in the arc. A long arc lets air in, and oil, rust, paint, mill scale and zinc all add gas of their own. Wind or a draught across the arc strips the shielding away, which matters when you weld outdoors on a gate or a fence.

The fixes are simple. Store rods dry in a closed box or tin, away from the wall in the rainy season. Follow the packet if it calls for drying a rod. Grind or wire-brush the joint back to bright metal for a few centimetres either side. Shorten the arc until it is about the width of the core wire, and slow down a little. Shield the work from wind with a board or sheet. If you cannot stop pinholes, cut the weld out and redo it, because a porous weld is weaker than it looks and a leaking one is useless on a tank or trough.

Why Is There So Much Spatter?

Spatter is the small balls of metal thrown out around the weld. A little is normal with some rods. A lot means the arc is too violent or the rod is not right. The causes are current too high, a long arc, damp rods and dirty metal. Spatter does not weaken a good weld by itself, but it burns skin, ruins paint and sticks to the plate, and it is often a warning that something else is wrong.

Lower the current by a small step and look again, shorten the arc and swap to a dry rod. If the spatter is gone, you had found the cause. If a good rod, a short arc and the right current still spatter badly, check that the earth clamp is on clean metal and that the supply is stable. Our guide to running a welding machine on a generator or inverter explains how an undersized source makes the arc ragged.

What Is Undercut, and Why Does It Break Gates?

Undercut is a groove melted into the plate along the edge of the weld and left unfilled. It looks like a thin trench beside the bead. It matters because the groove makes a notch, and notches are where cracks start under repeated load. This is why hinges, trailer drawbars and hooks so often fail at the toe of a weld rather than in the middle.

The causes are too much current, an arc that is too long, travelling too fast, and holding the rod at a wrong angle so the heat digs into one side. If you weave, pausing at the edges helps fill the groove. The fixes: lower the current, shorten the arc, slow down slightly, and angle the rod so it splits the heat between both plates. Look at the edge of every bead with the light low across it, because undercut hides in flat light.

A good-looking bead can still be weak. A weld that sits on top of the plate without melting into it looks acceptable and carries almost nothing. Look at the edges, not just the top, and test a scrap made with the same settings before you trust a weld that carries a load.

What Are Lack of Fusion and Slag Inclusions?

Lack of fusion means the weld metal has not melted into the plate or the previous pass. The bead sits on the surface with a sharp line where it meets the plate, like glue laid on top. The causes are current too low, travelling too fast, a rod too large for the joint, a wrong angle and dirty or oxidised surfaces. The fix is to raise the current, slow the travel, aim the arc at the root of the joint and clean the metal. On thicker plate, leave a small gap or bevel the edges so the arc can reach the bottom.

Slag inclusions are pieces of slag trapped inside or beside the weld, seen as dark lines or patches. The usual causes are not chipping and brushing the slag off between passes, current too low to float the slag out, and a joint too narrow for the rod to work in. The fix is to chip every pass clean, use enough current, and open up a narrow joint. A wire brush and a chipping hammer cost little compared with a weld that fails.

Why Do Welds Crack, Burn Through or Come Out Wavy?

Cracks. Small star-shaped cracks at the end of a bead are crater cracks, caused by breaking the arc abruptly. Pause at the end of a run to fill the crater before lifting off. Longer cracks along or across a weld are more serious. The usual suspects are hard or unknown steel such as leaf spring, some rebar or cast iron, cooling too quickly, a rigid joint with no room to move, and damp low-hydrogen rods. Do not weld on hard steel or cast iron as if it were mild steel. Find out what the metal is, use a rod made for it, and ask a qualified welder about warming the part first.

Burn-through. On thin sheet, such as a trough or a roof gutter, too much current or too slow a travel melts a hole. Lower the current, use a smaller rod, travel a little faster and weld in short stitches so the heat can spread. Our guide to rust protection for welded steel is the right next step once the weld is sound.

A wavy, uneven bead. The causes are an arc length that keeps changing, an unsteady hand, an awkward body position, and a dirty or wrong-shade lens that hides the pool. Brace both elbows, set the work at a comfortable height, move your whole arm rather than just the wrist, and practise a straight line on scrap until the ripples are even.

Which Cause Matches Which Defect?

Most defects have more than one cause, but a few causes appear again and again. The grid below shows the usual pattern, so you can work backward from what you see to the settings or habits to check first.

Defects and their usual causes Work Backward From the Defect Illustrative: the common pattern, not a count of real welds Amps high Amps low Too fast Long arc Damp rod Dirty metal Slag left Porosity Spatter Undercut Lack of fusion Slag inclusion Burn-through
Illustrative summary of the causes commonly listed for each defect in welding guides such as those from ESAB and the Welding Technology Institute of Australia. A dot means the cause is a usual suspect; real welds often have more than one.
What you seeMost likely causesFirst fix to try
Pinholes, foamy beadDamp rod, long arc, dirty or coated metalDry rod, shorter arc, grind to bright metal
Heavy spatterCurrent too high, long arc, damp rodLower current, shorten arc, change rod
Groove along the edgeCurrent too high, long arc, too fastLower current, slow down, adjust angle
Bead sits on top, no melt-inCurrent too low, too fast, wrong angleRaise current, slow down, aim at the root
Dark lines or patchesSlag not cleaned, current too lowChip and brush every pass
Hole in thin sheetCurrent too high, travelling too slowlyLower current, smaller rod, stitch weld
CracksHard steel, cooling too fast, abrupt arc break, damp low-hydrogen rodIdentify the steel, fill the crater, ask a qualified welder

How Do I Test a Weld Without Special Equipment?

A workshop test is not certification, but it is far better than hoping. Make a small test piece with the same rod, current and position as the real job. Then try one of these two simple checks.

The break test. Weld two pieces of flat bar in a T shape with a fillet weld on one side. Clamp the upright in a vice and hammer the plate over until it breaks or folds flat. A sound weld tears the parent metal or bends flat without the weld coming away. If the weld peels off cleanly, shows holes or slag lines in the break face, or has silver patches where it never fused, change your settings and make another.

The bend test. Weld two flat plates edge to edge, grind the weld flush, clamp in a vice and bend the joint over with a hammer. A good weld bends without a crack opening across the face of the bend. A crack means lack of fusion or a cracking problem to fix before the job.

Both tests suit gates, frames, tables and feeders. They are not enough for anything that carries people, lifts loads or holds pressure, such as a trailer hitch, a crane hook or a pressure tank. For those, use a certified welder and proper inspection.

What Safety Do I Need for Stick Welding?

Defects are about quality, but the same habits protect your body. The arc gives off ultraviolet light strong enough to burn the eye without pain at the time, with the damage arriving hours later. Use a proper helmet with the right shade filter, a screen to protect helpers and bystanders, and clear glasses when chipping slag. Our farm and workshop safety guide explains the shade numbers and the rest of the kit.

Welding fume is not for breathing. Keep your head out of the plume, weld in the open or with ventilation, and never weld inside a closed tank. Galvanised steel is a special case: burning off the zinc coating gives off fume that can cause metal fume fever, with flu-like symptoms. Grind the coating back before you weld and ventilate well. Never weld a drum or tank that has held fuel, oil or chemicals, because the vapour can explode. Keep gloves and clothing dry, clear anything that burns from the bay, and check the cable insulation and earth clamp before every session.

Where to Find Welding Equipment

Fuga serves workshops from six branches across Kenya, and our team can talk through the right machine, rods and helmet for your work. Our product list does not currently show a named arc welding machine page, so message the team on WhatsApp to ask what is available at your nearest branch. Browse the wider range under workshop and industrial tools.

Next time a weld looks wrong, resist the urge to turn the dial. Read the bead, name the defect, pick the likely cause from the table, change one thing and test a scrap. That habit costs a few minutes and saves the weld, the gate and the customer.

Key Takeaways

  • Most stick welding defects trace to six causes: current too high or too low, travelling too fast, a long arc, damp rods, and dirty or coated metal.
  • Porosity is trapped gas: dry your rods, shorten the arc and grind to bright metal. Undercut and spatter often mean the current is too high.
  • Lack of fusion and slag inclusions usually mean the current is too low or the travel too fast, and the slag was not cleaned between passes.
  • Change one thing at a time and test a scrap made with the same settings before you weld the real job.
  • A break test or bend test in a vice is a good workshop check, but it is not enough for lifting, pressure or anything that carries people.
  • Use a proper helmet and shade, ventilate, grind off galvanising before welding, and never weld a drum that held fuel.

Frequently Asked Questions

Why does my weld have small holes in it?

Small holes are porosity, gas trapped as the weld froze. The usual causes are damp rods, a long arc, rust, oil, paint or zinc on the metal, wind blowing across the arc, and travelling too fast. Dry the rods, clean to bright metal and shorten the arc.

What causes undercut when welding?

Undercut is a groove melted into the plate beside the weld. It is caused mainly by current set too high, a long arc, travelling too fast and a wrong rod angle. Lower the current, shorten the arc, slow down and angle the rod to share the heat between the plates.

Why does my weld sit on top and not stick to the plate?

That is lack of fusion. The current is usually too low, the travel too fast, the rod too big for the joint, or the metal dirty. Raise the current, slow down, aim the arc at the root and clean the joint. Such a weld can look fine and carry almost nothing.

How can I test my welds without special equipment?

Make a test piece with the same rod and settings. For a fillet weld, clamp it in a vice and hammer it over to see whether the weld fractures cleanly with holes or slag lines. For a butt weld, grind it flush and bend it over to look for cracks. Both are workshop checks, not certification.

Is it safe to weld galvanised steel?

Burning off zinc releases fume that can cause metal fume fever, with flu-like symptoms. Grind the coating back before welding, work in the open or with strong ventilation, and keep your head out of the plume. Never weld a drum or tank that has held fuel or chemicals.